Causes of External Folds and Indentations in Hot-Rolled Seamless Steel Pipes

Oct 15, 2025

Leave a message

External Folds

 

Defect Characteristics:

① Regular folds on the surface of the steel pipe, such as triangular, double-seam straight, single-seam straight, or irregular sheet-like folds.

② A fold on the longitudinal surface of the steel pipe, typically continuous or intermittent, resembling a sewing machine stitch, or staggered at 60°, 120°, or 180°.

③ Spiral folds on the longitudinal surface of the steel pipe.

④ A continuous dotted or short oblique line fold on the longitudinal surface of the steel pipe, with two or three staggered 120° lines in severe cases.

 

Hot rolled seamless steel pipe for sale

 

Causes:

① Spiral folds are caused by longitudinal cracks on the tube surface, severe inclusions, shrinkage holes, or other factors.

② Poor surface cleaning of the tube surface, sharp edges, or warping.

③ Nodules on the piercing machine guide plate or scratches on the piercing machine outlet nozzle. ④ Cracks or bruises on the continuous rolling mill or the stretch-reducing rolls.

⑤ The chamfering of the stretch-reducing rolls does not meet requirements, the rolls have exceeded their service life, or the new and old mill frames are improperly used.

⑥ Mechanical abrasions or bruises during the conveying of the steel pipes from the stretch-reducing mill.

⑦ Insufficient or no cooling water for the stretch-reducing rolls causes the stretch-reducing rolls to stick to the steel.

 

Indentation

Defect characteristics: Random or regular localized indentations and chippings appear on the longitudinal surface of the steel pipe. Shapes may include nuclei, stripes, transverse indentations, warping, cracks, or iron filings.

 

Causes:

① Metal objects adhere to the surface of the rolls in the stretch-reducing mill's finished product stand.

② Scars or other foreign matter press against the steel pipe surface and break off.

③ Bumps or scratches on the hot steel pipe.

④ Bumps or indentations caused by the transverse movement or sawing device.

 

Judgment:

General pipes: For wall thickness ≤ 8mm, the indentation depth shall not exceed 90% of the negative deviation. For wall thickness > 8mm, the indentation depth shall not exceed 80% of the negative deviation. The maximum depth shall not exceed 1.0mm.

Boiler pipes: The indentation depth shall not exceed half of the negative deviation of the wall thickness, with a maximum of 0.6mm.

Oil casing and tubing: The indentation depth shall not exceed half of the negative deviation of the wall thickness. For S ≥ 10mm, the maximum depth shall not exceed 0.6mm. For S < 10mm, the maximum depth shall not exceed 0.5mm.

Send Inquiry